Right after I made my previous post, I went and developed a test strip of 35 mm Tri-X 400 in PMK (pyro) developing it for 20 minutes at 70 degrees without agitation. This is supposed to be a no-no. However, it worked just fine, giving me full scale negs with plenty of stain without a sign of uneven development. I'll send some stuff to Ed when I can get to the post office. I don't think I could show what I want to show by e-mail.(posted 8170 days ago)