Hardening the emulsion and applying modest heat helps to get a nicer gloss. There is no need to ferrotye. I suggest hardening after fixing and washing, since this will not prolong the washing times. Use a hardener based on potassiumaluminiumsulfate (40g to 100g in 1 Liter is the minimal version of a hardening solution which non the less works well -- Potassiumchromiumsulfate will work too) and give it a 10 minute wash to remove the solution from the paper base. Formaldehyde hardeners are even more effective, but I cannot suggest them due to health risks. Use a drying press and put the prints on face up -- towards the cloth! Apply modest heat until they are dry. Even without the heat the hardened emulsion will have significantly more gloss and shine, but the heat helps.(posted 8222 days ago)